Question

What is the critical zone on a tank bottom?

The critical zone is the part of the tank bottom or annular plate within three inches of the inside edge of the shell, measured radially inward (API 653 clause 3.11). It is the strip of plate that carries the shell’s load into the bottom, so API 653 gives it its own minimum thickness and tighter repair rules than the rest of the floor.

Minimum thickness in the critical zone

Clause 4.4.5.4: unless a stress analysis is done, the critical zone plate at the next inspection must be at least the smaller of three millimeters, just under an eighth of an inch (half the API 650 bottom plate thickness, not counting corrosion allowance), and half of the lower shell course t-min from clause 4.3.3.1, and never less than a tenth of an inch. Averaging bottom thickness is not permitted.

Isolated pitting and isolated corroded areas may not affect the zone’s strength. For those, the minimum at the next internal inspection may come from Table 4.4 or an RBI (risk-based inspection) assessment instead, but only after the storage tank engineer decides the zone’s structural integrity is not affected, which may take an engineering evaluation (see clause 4.3.3.6).

How wide is the critical zone?

Three inches (seventy-five millimeters), measured radially inward from the inside of the shell. It is not the whole annular ring, and it is not the outside projection of the bottom past the shell, which has its own minimum under clause 4.4.5.7.

Repairs in the critical zone

  • No welding or weld overlay in the zone except on widely scattered pits, pinholes, cracks in the bottom plate, the shell-to-bottom weld, welded-on patch plates, or where the bottom plate welded to the shell is being replaced (clause 9.11.1.2.1).
  • Corroded plate in the zone is repaired only by pit welding or overlay welding, within the limits of clause 9.11.1.6.
  • Welded-on patch plates are allowed under clause 9.11.1.2: no thicker than one quarter inch, tombstone shaped within six inches of the shell, two-pass perimeter welds, no patch on a patch, no butt-welding to an existing patch, and no longer than twenty-four inches along the shell. They are not allowed when the bottom runs above two hundred degrees Fahrenheit for carbon steel or one hundred degrees Fahrenheit for stainless steel.
  • Anything beyond that: cut out the bottom plate welded to the shell and install a new one, replacing the shell-to-bottom weld at least twelve inches each side (clause 9.11.1.2.4). A welded-on patch plate that does not meet those requirements may be used only if an engineer experienced in API 650 tank design reviews and approves the repair method (clause 9.11.1.3).
  • Sumps in the zone follow the same rules (clause 9.11.1.5).

Examination

The root and final pass of a welded-on patch plate weld in the critical zone are visually examined and examined by magnetic particle or liquid penetrant over their full length (clause 12.1.7.2).

Edition note: in API 653 Fifth Edition, Addendum 4, the definition is clause 3.11. Some clauses (4.4.5.4, 9.11.1.2, 12.1.7.2) still say "see 3.10", which is now the corrosion rate definition.

Also asked as

What is the API 653 critical zone definition?

Clause 3.11: the portion of the tank bottom or annular plate within three inches of the inside edge of the shell, measured radially inward.

What repairs are allowed in the critical zone?

Pit welding and overlay welding within the limits of clause 9.11.1.6, welded-on patch plates within the limits of clause 9.11.1.2, and replacement of the bottom plate welded to the shell. A welded-on patch plate that does not meet those requirements may be used only if an engineer experienced in API 650 tank design reviews and approves the repair method (clause 9.11.1.3).

TankForge is API 653 inspection software built by a working API 653 inspector. Draft report. Your certified inspector reviews and signs.